如何讓舊环氧地坪顏值再現的問題給我們做瞭詳細介紹,其實不管是新环氧地坪還是舊环氧地坪,顏值和質量肯定是我們做關心的,尤其是新做的环氧地坪。經常會有客戶咨詢剛施工好的环氧地坪因為施工环境的不同經常會或多或少的出現一些影響环氧地坪顏值和質量的問題,其中环氧地坪廠傢小編就以下四種常見的問題給大傢進行詳細介紹,在此也提醒施工人員能夠規范施工要求,避免類似問題的發生。
How to make the old epoxy floor color reproduction problem gives us a detailed introduction, in fact, whether it is new or old floor, the color and quality must be our concern, especially the new epoxy floor. Customers often consult newly constructed epoxy flooring because of the different construction environment, there are more or less problems affecting the appearance and quality of epoxy flooring. The epoxy flooring manufacturer's small edition gives you a detailed introduction of the following four common problems, which also reminds the constructors to standardize the construction. Avoid similar problems. 一、發白
One, white
原因:1、冬天油漆反應速度過慢,用硬化劑與空氣反應產生白霧狀;2、在低溫多濕之場合施工;3、施工後遭水侵入。
Reasons: 1. The reaction speed of paint is too slow in winter, and the reaction between hardener and air produces a white fog; 2. Construction in low temperature and humidity occasions; 3. Water intrusion after construction.
預防方法:1、選擇適當硬化劑;2、避免低溫多濕條件施工,不得已時采取加溫除濕措施,如空調加溫降濕,暖風機加溫;3、避免施工後有水侵入。
Preventive methods: 1. Choose appropriate hardener; 2. Avoid construction under low temperature and humidity conditions, take heating and dehumidification measures when necessary, such as air conditioning he印花地坪ating and cooling, warm air heating; 3. Avoid water intrusion after construction.
二、色差
Two, color difference
原因:1、环氧樹脂地坪塗料主劑沉淀,未充分攪拌均勻;2、倒料在地面上,與前接縫處之接觸時間過久;3、塗層厚薄不均勻;4、施工中途斷料;5、采用不同批號面漆。
Reasons: 1. Sedimentation of main agent of epoxy resin floor coatings and insufficient mixing uniformity; 2. Over-long contact time between poured material and front joint on the ground; 3. uneven thickness of coatings; 4. Broken material during construction; 5. Different batches of topcoats.
預防方法:1、施工前主劑應先充分攪拌均勻;2、避免與前接縫處接觸間隔太久,盡可能整個操作線一起施工;3、盡量適用固定工具及加強施工人員施工熟練度;4、塗料須一次備足,防止斷料;5、盡可能使用同一批號塗料。
1. Before construction, the main agent should be fully stirred evenly; 2. Avoid long contact interval with the front joint, and construct with the whole operation line as far as possible; 3. Apply fixing tools as far as possible and strengthen the construction skillfulness of the builders; 4. Coatings should be prepared at one time to prevent material breakage; 5. Use the same batch of coatings as possible.
三、起水泡
Three. Blister
原因:1)結構體地下層、水箱旁、底樓層或其它地面水氣濕度偏高;2)沒做斷水處理或底漆封閉不良。
Reasons: 1) high moisture content of water and air in the basement, near the water tank, bottom floor or other surface of the structure; 2) no water treatment or poor sealing of primer.
預防方法:1、施工前先以水份計協助判斷;2、水份及水壓太高的地點須先做斷水處理;3、選擇親水性的环氧樹脂底漆。
Preventive methods: 1. Use moisture meter to help judge before construction; 2. Water cut-off treatment should be done at places with high water content and pressure; 3. Select hydrophilic epoxy resin primer.
四、火山口
Four. Crater
原因:1、下層有坑洞;2、下層有油污;3、塗料本身原因。
Reasons: 1, there are potholes on the lower level; 2, there are oil pollution on the lower level; 3, the reasons for the coating itself.
預防方法:1、施工前先用环氧批土把坑洞修補平後再進行施工;2、將下層油污清除幹凈;3、先用合適的塗料。
Preventive methods: 1. Use epoxy batch soil to repair the pit before construction; 2. Clean up the oil contamination in the lower layer; 3. Use appropriate paint first.
關於影響环氧地坪質量的因素及預防措施據暫時給大傢介紹到這裡,其實环氧地坪的施工是一件比較嚴格的工程,一旦出現問題影響的不僅是返工重修這麼簡單,更重要的是耗費大量的財力影響企業的生產效率,因此建議大傢對於环氧地評的施工一定要找專業的施工團隊,確保最終的效果。
The factors that affect the quality of epoxy flooring and preventive measures are briefly introduced here. In fact, the construction of epoxy flooring is a more stringent project. Once problems arise, it is not环氧地坪 only simple to rework and repair, but more importantly, it costs a lot of money to affect the production efficiency of enterprises. Therefore, we suggest that you For the construction of epoxy rating, we must find professional construction team to ensure the final effect.